Pigment and binder

Pigment Volume Concentration (PVC) and Pigment Weight Concentration (PWC)

Published by Morex Technologies ·

Pigment volume concentration (PVC) is the volume of pigment and extender as a percentage of the total volume of the dry film (pigment plus binder solids). Pigment weight concentration (PWC) expresses the pigment share by weight instead of volume.

The PVC formula

PVC (%) = Vp ÷ (Vp + Vb) × 100

SymbolMeaningUnit
VpVolume of all pigments and extenders (weight ÷ density)cm³
VbVolume of the binder solids (binder solid weight ÷ solid density)cm³

PVC is a dry-film property: water and solvents are not part of either volume. Non-volatile additives are often small enough to ignore, but if they are significant include them in Vb.

Worked example

Illustrative water-based formulation, 100 g basis
Raw materialWeight (g)Density (g/cm³)Solids (% w/w)Solid density (g/cm³)
Acrylic emulsion (binder)301.05501.15
Titanium dioxide, rutile (pigment)204.101004.10
Calcium carbonate (extender)152.701002.70
Water351.000—
Total100

Vp = 20 ÷ 4.10 + 15 ÷ 2.70 = 4.878 + 5.556 = 10.434 cm³. Vb = (30 × 0.50) ÷ 1.15 = 13.043 cm³. PVC = 10.434 ÷ (10.434 + 13.043) × 100 = 44.44 %.

Example values are illustrative, chosen to show the arithmetic. Use the density, solids and oil absorption from your own raw materials’ technical data sheets.

The PWC formula and its two conventions

PWC (%) = Wp ÷ (Wp + Wb) × 100

SymbolMeaningUnit
WpWeight of all pigments and extendersg
WbWeight of the binder solidsg

This dry-film form is the weight counterpart of PVC. For the example, PWC = 35 ÷ (35 + 15) × 100 = 70.0 %. Some data sheets instead quote pigment content as a percentage of the total wet paint weight (35 % in the example). Always state which basis you are using; the two figures are not interchangeable.

Converting PWC to PVC

PVC = (PWC ÷ ρp) ÷ [ PWC ÷ ρp + (100 − PWC) ÷ ρb ] × 100

SymbolMeaningUnit
PWCDry-film pigment weight concentration%
ρpDensity of the pigment blend (total pigment weight ÷ total pigment volume)g/cm³
ρbDensity of the binder solidsg/cm³

In the example the pigment blend density is 35 ÷ 10.434 = 3.355 g/cm³ and ρb = 1.15 g/cm³. With PWC = 70 %: (70 ÷ 3.355) ÷ (70 ÷ 3.355 + 30 ÷ 1.15) × 100 = 44.44 %, the same PVC as before.

Effect of TiO₂ and filler changes

Increasing titanium dioxide in the example from 20 g to 25 g raises Vp to 6.098 + 5.556 = 11.654 cm³ and PVC to 47.19 %, while dry-film PWC rises to 40 ÷ 55 × 100 = 72.73 %. Because extenders are usually less dense than TiO₂, replacing TiO₂ with the same weight of extender raises PVC more than it raises PWC.

How PVC affects paint properties

As PVC rises, gloss generally falls, because more pigment particles reach the film surface. Below the critical pigment volume concentration (CPVC) the binder fills the spaces between particles; above it the film contains air voids, which typically increases porosity and reduces scrub and stain resistance. That is why PVC is read together with CPVC.

Common calculation mistakes

  • Calculating PVC with wet-paint volume instead of dry-film volume.
  • Using the liquid resin’s weight and density for binder volume instead of its solids.
  • Mixing the two PWC conventions when comparing formulations.
  • Leaving a colour pigment out of the pigment volume because it is classified differently from extenders.

Frequently asked questions

What is the difference between PWC and PVC?

PWC is the pigment share by weight and PVC the pigment share by volume of the dry film. Dense pigments such as TiO₂ make PWC much higher than PVC.

How do I calculate PVC using pigment and binder volumes?

Divide each pigment’s weight by its density and add them for Vp; divide the binder solid weight by its solid density for Vb; then PVC = Vp ÷ (Vp + Vb) × 100.

How do I calculate pigment volume from pigment weight and specific gravity?

Divide the weight in grams by the specific gravity (numerically equal to density in g/cm³) to get the volume in cm³.

How do extenders affect PVC?

Extenders add pigment volume, so they raise PVC. Their lower density means a given weight of extender adds more volume than the same weight of TiO₂.

Calculating this in PaintOS

PaintOS calculates total volume, SVR, NVW, VMC, PVC and an estimated CPVC from the density, solids, solid density and oil absorption stored for each raw material, and recalculates them as a formulation changes.

Learn about PaintOS formulation management →